02.06.15
Phase A | |
SP-422P (Strahl & Pitsch) (Beeswax) | 10.00 |
SP-63 (Strahl & Pitsch) (Carnauba (copernicia cerifera) wax) | 4.00 |
Lexemul 5151 (Inolex) (Glyceryl stearate) | 2.00 |
Lexorez 2001 (Inolex) (Trimethylpentanediol/adipic acid/glycerin crosspolymer) | 8.00 |
Ganex V-220 (PVP/Vp eicosense copolymer) | 5.00 |
Phase B | |
LexFeel N5 (Inolex) (Diheptyl succinate and) capryloyl glycerin/sebacic acid copolymer) | 52.50 |
Bentone 38V (Elementis) (Disteardoimonium hectroite) | 5.00 |
Propylene carbonate | 1.00 |
Phase C | |
Unipure Black, LC989 (Sensient Technologies) (iron oxide) | 10.00 |
CI77007 (Ultramarines Blue) | 1.00 |
Mica sericite | 0.50 |
Phase D | |
Lexgard GMCY (Inolex) (Glyceryl caprylate) | 1.00 |
Procedure | |
Combine phase A ingredients, heat to 85°C and mix until uniform. Disperse phase C pigments into phase B and begin homogenizing until smooth. Add phase D to combined phase “B/C”. Mix until uniform. Heat batch to 85°C and add phase A with propeller mixing. Cool batch to 35°C. | |
Properties | |
Viscosity @ 25°C (Brookfield RVT; Spindle T-D @ 10 rpm)—30,000cps. | |
More Information | |
Inolex, Inc. 215-271-0800 Fax: 215-271-2621 www.inolex.com |